France AFNOR 1.4301 Austenite and 1.4301 Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
| Category | Type | Steel Grade | Standard | Country | Application | 
|---|---|---|---|---|---|
| Steel Grades | Special Steel | 1.4301 | AFNOR | France | Austenite | 
| 1.4310 | |||||
| 1.4318 | |||||
| X2CrNiN18-7 | |||||
| X2CrNi18-9 | |||||
| 1.4307 | |||||
| X2CrNi19-11 | |||||
| 1.4306 | |||||
| X2CrNiN18-10 | |||||
| 1.4311 | |||||
| X2CrNi18-10 | 
| C(%) | Si(%) | Mn(%) | P(%) | S(%) | Cr(%) | Ni(%) | N(%) | 
|---|---|---|---|---|---|---|---|
| Max 0.07 | Max 1.00 | Max 2.00 | Max 0.045 | Max 0.015 | 17.00-19.50 | 8.00-10.50 | Max 0.11 | 
| Yield Rp0.2 (MPa) | Tensile Rm (MPa) | Impact KV/Ku (J) | Elongation A (%) | Reduction in cross section on fracture Z (%) | As-Heat-Treated Condition | Brinell hardness (HBW) | 
|---|---|---|---|---|---|---|
| 936 (≥) | 211 (≥) | 22 | 42 | 22 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 431 | 
| Temperature (°C) | Modulus of elasticity (GPa) | Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) | Specific thermal capacity (J/kg·°C) | Specific electrical resistivity (Ω mm²/m) | Density (kg/dm³) | Poisson’s coefficient, ν | 
|---|---|---|---|---|---|---|---|
| 33 | - | - | 0.21 | - | |||
| 879 | 148 | - | 41.3 | 114 | - | ||
| 551 | - | 14 | 11.2 | 242 | 322 | 
Heat treated : 1113°C - 1893°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com