1.2326 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
| Category | Type | Steel Grade | Standard | Country | Application | 
|---|---|---|---|---|---|
| Steel Grades | Mould Steel | 1.2326 | |||
| 1.1168 | |||||
| GS-40Mn5 | |||||
| 1.1168 | |||||
| GS-C25S | |||||
| 1.1339 | |||||
| GX165CrV12 | |||||
| 1.2201 | |||||
| G60CrMoV10-7 | |||||
| 1.2320 | |||||
| G48CrMoV6-7 | 
| C ≤ | Si ≤ | Mn ≤ | P ≤ | S ≤ | Cr | Ni | 
|---|---|---|---|---|---|---|
| 0.40-0.50 | 0.15-0.35 | 0.60-0.90 | 0.030 | 0.030 | 1.30-1.60 | |
| Mo | Al | Cu | Nb | Ti | V | Ce | 
| 0.65-0.85 | 0.25-0.35 | |||||
| N | Co | Pb | B | Other | ||
| Yield Rp0.2 (MPa) | Tensile Rm (MPa) | Impact KV/Ku (J) | Elongation A (%) | Reduction in cross section on fracture Z (%) | As-Heat-Treated Condition | Brinell hardness (HBW) | 
|---|---|---|---|---|---|---|
| 271 (≥) | 858 (≥) | 21 | 43 | 23 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 333 | 
| Temperature (°C) | Modulus of elasticity (GPa) | Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) | Specific thermal capacity (J/kg·°C) | Specific electrical resistivity (Ω mm²/m) | Density (kg/dm³) | Poisson’s coefficient, ν | 
|---|---|---|---|---|---|---|---|
| 32 | - | - | 0.32 | - | |||
| 291 | 232 | - | 21.3 | 312 | - | ||
| 819 | - | 21 | 12.2 | 414 | 233 | 
Heat treated : 1738°C - 1286°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com