China GBT GH4099 wrought Fe/Ni-base superalloy and GH4099 Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
| Category | Type | Steel Grade | Standard | Country | Application | 
|---|---|---|---|---|---|
| Steel Grades | Special Alloy | GH4099 | GBT | China | wrought Fe/Ni-base superalloy | 
| GH3600 | |||||
| GH3625 | |||||
| GH3652 | |||||
| GH4033 | |||||
| GH4037 | |||||
| GH4049 | |||||
| GH4080A | |||||
| GH4090 | |||||
| GH4093 | |||||
| GH4098 | 
| C(%) | Si(%) | Mn(%) | P(%) | S(%) | Cr(%) | Ni(%) | Mo(%) | V(%) | W(%) | Cu(%) | Co(%) | B(%) | Al(%) | Ti(%) | Mg(%) | Fe(%) | 
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| ≤0.08 | 0.50 | 0.40 | 0.015 | 0.015 | 17.00-20.00 | Bal | 3. 50-4. 50 | - | 5.00-7.00 | . | 5.00-8.00 | ≤0.005 | 1.70-2. 40 | 1.00 -1.50 | ≤0.010 | ≤2.00 | 
| Yield Rp0.2 (MPa) | Tensile Rm (MPa) | Impact KV/Ku (J) | Elongation A (%) | Reduction in cross section on fracture Z (%) | As-Heat-Treated Condition | Brinell hardness (HBW) | 
|---|---|---|---|---|---|---|
| 459 (≥) | 263 (≥) | 14 | 11 | 33 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 344 | 
| Temperature (°C) | Modulus of elasticity (GPa) | Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) | Specific thermal capacity (J/kg·°C) | Specific electrical resistivity (Ω mm²/m) | Density (kg/dm³) | Poisson’s coefficient, ν | 
|---|---|---|---|---|---|---|---|
| 44 | - | - | 0.14 | - | |||
| 724 | 889 | - | 22.3 | 312 | - | ||
| 169 | - | 42 | 31.2 | 441 | 433 | 
Heat treated : 1852°C - 1691°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com