SCS32 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
| Category | Type | Steel Grade | Standard | Country | Application | 
|---|---|---|---|---|---|
| Steel Grades | Mould Steel | SCS32 | |||
| SCS18 | 
                                |||||
| SCS19 | 
                                |||||
| SCS19A | 
                                |||||
| SCS20 | 
                                |||||
| SCS21 | 
                                |||||
| SCS21X | 
                                |||||
| SCS22 | 
                                |||||
| SCS23 | 
                                |||||
| SCS24 | 
                                |||||
| SCS31 | 
                                
| 
				C ≤  | 
			
				Si ≤  | 
			
				Mn ≤  | 
			
				P ≤  | 
			
				S ≤  | 
			Cr | Ni | 
|---|---|---|---|---|---|---|
| 0.03 | 1.0 | 1.5 | 0.035 | 0.025 | 25-27 | 4.5-6.5 | 
| Mo | Al | Cu | Nb | Ti | V | Ce | 
| 2.5-3.5 | 2.5-3.5 | |||||
| N | Co | Pb | B | Other | ||
| 0.12-0.25 | ||||||
| Yield Rp0.2 (MPa)  | 
                                            Tensile Rm (MPa)  | 
                                            Impact KV/Ku (J)  | 
                                            Elongation A (%)  | 
                                            Reduction in cross section on fracture Z (%)  | 
                                            As-Heat-Treated Condition | Brinell hardness (HBW) | 
|---|---|---|---|---|---|---|
| 676 (≥) | 164 (≥) | 44 | 14 | 21 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 342 | 
| Temperature (°C)  | 
                                        Modulus of elasticity (GPa)  | 
                                        Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C)  | 
                                        Specific thermal capacity (J/kg·°C)  | 
                                        Specific electrical resistivity (Ω mm²/m)  | 
                                        Density (kg/dm³)  | 
                                        Poisson’s coefficient, ν | 
|---|---|---|---|---|---|---|---|
| 22 | - | - | 0.14 | - | |||
| 898 | 985 | - | 11.3 | 242 | - | ||
| 151 | - | 44 | 34.2 | 121 | 214 | 
Heat treated : 1546°C - 1272°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com