1.3964 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
| Category | Type | Steel Grade | Standard | Country | Application |
|---|---|---|---|---|---|
| Steel Grades | Mould Steel | 1.3964 | |||
| 1.3802 |
|||||
| G-X25MnCrNi8-8-6 |
|||||
| 1.3966 |
|||||
| G-X12CrNi18-11 |
|||||
| 1.3955 |
|||||
| G-X2CrNi18-13 |
|||||
| 1.3940 |
|||||
| G-X2CrNiMoN18-14 |
|||||
| 1.3952 |
|||||
| G-X2CrNiMnMoNb21-16-5-3 |
|
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
|---|---|---|---|---|---|---|
| 0.030 | 1.00 | 4.00-6.00 | 0.025 | 0.010 | 20.0-21.5 | 15.0-17.0 |
| Mo | Al | Cu | Nb | Ti | V | Ce |
| 3.00-3.50 | ≤0.25 | |||||
| N | Co | Pb | B | Other | ||
| 0.25-0.35 | ||||||
| Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
|---|---|---|---|---|---|---|
| 246 (≥) | 264 (≥) | 21 | 32 | 41 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 243 |
| Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
|---|---|---|---|---|---|---|---|
| 43 | - | - | 0.11 | - | |||
| 521 | 544 | - | 13.3 | 121 | - | ||
| 722 | - | 32 | 41.2 | 341 | 424 |
Heat treated : 1669°C - 1123°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com