Available 24/7 at contact@steel-grades.com

X12CrNi17-7

Description

International ISO ISO 6931-2, X12CrNi17-7 Specialsteel Stainless steels for springs - Part 2: Narrow strip and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.

Datasheet for: Steel Grades:Specialsteel: X12CrNi17-7
Category Class Grade Standard Country Application
Steel GradesSpecialsteel X12CrNi17-7 ISO International Stainless steels for springs - Part 2: Narrow strip

Chemical composition(mass fraction)(wt.%) of the X12CrNi17-7

C Si Mn P S Cr Mo Ni
≤0.12 ≤1.50 ≤2.00 ≤0.045 ≤0.030 16.00 -18.00 ≤0.80 6.00 -9.00

Mechanical Properties of steel grade X12CrNi17-7

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV/Ku (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
752 (≥) 716 (≥) 21 43 33 Solution and Aging, Annealing, Ausaging, Q+T,etc 224

Physical Properties of steel grade X12CrNi17-7

Temperature
(°C)
Modulus of elasticity
(GPa)
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and Thermal conductivity
(W/m·°C)
Specific thermal capacity
(J/kg·°C)
Specific electrical resistivity
(Ω mm²/m)
Density
(kg/dm³)
Poisson’s coefficient, ν
31 - -     0.34 -  
398 112 - 32.3 231   -  
849 - 31 44.2   222 213

Heat Treatment of steel grade X12CrNi17-7

Heat treated : 1845°C - 1863°C

Technological Curves of steel grade X12CrNi17-7

Relevant standard of X12CrNi17-7

ISO 6931-2 Stainless steels for springs - Part 2: Narrow strip ISO-6931-2.pdf

Available Suppliers

Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...

Rfq.: sales@longhaisteel.com
  • Do you supply this X12CrNi17-7?
  • List your company on S&G now? Join
  • Non-paying users only
Top